Class: E330-16
AWS: A5.4
Conforms to Certification: AWS A5.4 ASME SFA A5.4
Weld Process: Shielded Manual Metal Arc
AWS Chemical Composition Requirements | |
C = 0.18 – 0.25 | Si = 0.90 max |
Cr = 14.0 – 17.0 | P = 0.04 max |
Ni = 33.0 – 37.0 | S = 0.03 max |
Mo = 0.75 max | Mn = 1.0 – 2.5 |
Cu = 0.75 max |
Application
E330-16 is a fully austenitic stainless steel electrode used to weld matching composition wrought and cast alloys. Generally used for resistance to oxidation at elevated temperatures.
Deposited Chemical Composition % (Typical) | ||
C = 0.21 | Cr = 15.40 | Ni = 34.10 |
Si = 0.50 | Mn = 1.95 | P = 0.021 |
S = 0.021 | Mo = 0.52 |
Deposited All Weld Metal Properties % | |
(Typical) As-Welded | |
Yield Strength | 85,000 psi |
Tensile Strength | 56,500 psi |
Elongation | 27% |
Deposited Charpy-V-Notch Impact Properties %
Not Applicable
Available Sizes & Recommended Welding Parameters | |||
Diameter | Voltage | Flat | Amperage Vertical & Overhead |
3/32 | 24-28 | 70-85 | 65-75 |
1/8 | 26-30 | 85-110 | 80-90 |
5/32 | 28-32 | 110-140 | 100-120 |
3/16 | 28-32 | 120-160 | 110-130 |