Class: ECoCr-C
AWS: A5.13
Conforms to Certification: AWS A5.13 ASME SFA A5.13
Class: ECoCr-C
Weld Process: Shielded Metal Arc
AWS Chemical Composition Requirements | |
C = 1.7 – 3.0 | Mo = 1.0 max |
Mn = 2.0 max | Fe = 5.0 max |
Si = 2.0 max | W = 11.0 – 14.0 |
Cr = 25 – 33 | Co = Remainder |
Ni = 3.0 max | Other = 1.0 max |
Available Sizes
3/32 x 14”
1/8 x 14”
5/32 x 14”
3/16 x 14”
1/4 x 14”
Application
Type #1 (ECoCr-C) is the highest hardness standard alloy in the group of cobalt alloys used for elevated temperature abrasive wear associated with corrosion. Deposits of this alloy have a large volume of chromium carbides that impact outstanding abrasive wear resistance. The addition of tungsten enhances high temperature hardness and matrix toughness for excellent adhesive and solid particle erosion wear resistance. It bonds well with all steels including stainless.
Deposited Chemical Compositon % (Typical) | |
C = 2.1 | Mo = 0.1 |
Mn = 0.1 | Fe = 2.3 |
Si = 0.9 | W = 12.1 |
Cr = 29.6 | Co = Balance |
Ni = 1.9 |
Deposited All Weld Metal Properties % (AW)
Hardness (2 layer) HRC 46 – 50
Deposited Charpy-V-Notch Impact Properties %
Not Applicable
Recommended Operation of Welding Rods
Flat Welding
Diameter | Amps DCEP |
1/8 | 90 – 120 |
5/32 | 135 – 180 |