Class: ER316H
AWS: A5.9
Conforms to Certification: AWS A5.9 ASME SFA A5.9
Weld Process Used for Tig (GTAW)
AWS Chemical Composition Requirements
C = 0.04 – 0.08
Cr = 18.0 – 20.0
Ni = 11.0 – 14.0
Mo = 2.0 – 3.0
Mn = 1.0 – 2.5
Si = 0.30 – 0.65
P = 0.03 max
S = 0.03 max
Cu = 0.75 max
Available Sizes
.030 x 36
.035 x 36
.045 x 36
1/16 x 36
3/32 x 36
1/8 x 36
3/16 x 36
5/32 x 36
Application
ER316H is used to weld wrought and cast forms of similar composition. The presence of molybdenum increases its creep resistance at elevated temperatures. The lower ferrite level of this nominal composition reduces the rate of corrosion in certain media and is suitable for use at cryogenic temperatures.
Deposited Chemical Composotion % (Typical) | ||
C = 0.06 | Mo = 2.25 | P = 0.012 |
Cr = 19.25 | Mn = 1.80 | S = 0.010 |
Ni = 11.25 | Si = 0.40 |
Mechanical Properties (R.T.) | |
Yield Strength | 59,000psi |
Tensile Strength | 88,000psi |
Elongation | 40% |
Reducation of Area | 60% |
Deposited All Weld Metal Properties
Data is typical for ER316H weld metal deposited by Tig using 100% Argon as the shielding gas.
Recommended Welding Parameters | |||
GTAW “Tig Process” | |||
Wire Diameter | Amps DCSP | Volts | Shielding Gas |
.035 | 60-90 | 12-15 | Argon 100% |
.045 | 80-110 | 13-16 | Argon 100% |
1/16 | 90-130 | 14-16 | Argon 100% |
3/32 | 120-175 | 15-20 | Argon 100% |
Note: Parameters for tig welding are dependent upon plate thickness and welding position.
Other shielding Gases may be used for Tig welding. Shielding gases are chosen taking Quality, Cost, and Operability into consideration.