Class: ENiCrMo-4
AWS: A5.11
Conforms to Certification: AWS A5.11 ASME SFA A5.11
Weld Process: Shielded Metal Arc Weld Process (SMAW)
AWS Chemical Composition Requirements | |
C = 0.02 max | Cu = 0.50 max |
Mn = 1.0 max | Ni = Remainder |
Fe = 4.0 – 7.0 | Co = 2.5 max |
P = 0.04 max | Cr = 14.5 – 16.5 |
S = 0.03 max | Mo = 15.0 – 17.0 |
Si = 0.20 max | W = 3.0 – 4.5 |
V = 0.35 max |
Please contact us for more information and availability
Application
ENiCrMo-4 (Alloy C276) is used for welding materials of similar composition. It can also be used for dissimilar welding between nickel base alloys and stainless steel, also for cladding applications.
Deposited Chemcial Composition % (Typical) | ||
C = 0.012 | Mn = 0.40 | Si = 0.14 |
Fe = 5.5 | Mo = 16.0 | W = 3.25 |
S = 0.004 | P = 0.012 | Cr = 15.5 |
Ni = 59.1 |
Deposited All Weld Metal Properties % (AW) | |
Tensile Strength | 105,000 psi |
Yield Strength | 79,000 psi |
Elongation | 38.5% |
Deposited Charpy-V-Notch Impact Properties %
Not applicable
Recommended Weld Parameters | Amperage (A) | ||
Diameter of Wire | Voltage (V) | Flat | Vertical and Overhead |
3/32 inches (2.4mm) | 24 – 28 | 70 – 85 | 65 – 75 |
1/8 inches (3.2mm) | 26 – 30 | 85 – 110 | 80 – 90 |
5/32 inches (4.0mm) | 28 – 32 | 110 – 140 | 100 – 120 |
3/16 inches (4.8mm) | 28 – 32 | 120 – 160 | 110 – 130 |