Class: ERNiCr-3
AWS: A5.14
Conforms to Certification: AWS A5.14 ASME SFA A5.14
Weld Process: GTAW Welding Process
AWS Chemical Composition Requirements | |
C = 0.10 max | Cu = 0.50 max |
Mn = 2.5 – 3.5 | Ni = 67.0 min |
Fe = 3.0 max | Co = 0.12 max |
P = 0.03 max | Ti = 0.75 max |
S = 0.015 max | Cr = 18.0 – 22.0 |
Si = 0.50 max | Cb/Ta = 2.0 – 3.0 |
Other = 0.50 max |
Available Sizes
.035 x 36
.045 x 36
1/16 x 36
3/32 x 36
1/8 x 36
5/32 x 36
Application
ERNiCr-3 (NA82) is used for welding Inconel alloy 600 and Incoloy 800, overlaying on steel and various dissimilar metal welding applications. Weld processes which can be used include GTAW, GMAW and ASAW.
Deposited Chemical Composition % (Typical) | ||
C = 0.03 | P = 0.003 | Ni = 72.9 |
Mn = 2.85 | S = 0.001 | Cr = 20.4 |
Fe = 1.1 | Si = 0.22 | Cb/Ta = 2.5 |
Deposited All Weld Metal Properties % (AW) | |
Tensile Strength | 85,500 psi |
Yield Strength | 52,500 psi |
Elongation | 38% |
Deposited Charpy-V-Notch Impact Properties %
Not applicable
Recommended Welding Parameters for TIG, MIG, and SAW Welding of Nickel Alloys | ||||
Process | Diameter of Wire | Voltage (V) | Amperage (A) | Gas |
Tig | .035 inches x 36 | 12 – 15 | 60 – 90 | 100% Argon |
.045 inches x 36 | 13 – 16 | 80 – 110 | 100% Argon | |
1/16 inches x 36 | 14 – 18 | 90 – 130 | 100% Argon | |
3/32 inches x 36 | 15 – 20 | 120 – 175 | 100% Argon | |
1/8 inches x 36 | 15 – 20 | 150 – 220 | 100% Argon |
Note: Other shielding Gases may be used for Tig welding. Shielding gases are chosen taking Quality, cost, and Operability into consideration.
Note: Both agglomerated and fused fluxes can be used for submerged arc welding.
Note: The chemical composition of the flux mainly affects the chemistry of the weld metal and consequently its corrosion resistance and mechanical properties.